Impact of M2-Hss Tool Pin Profile in FSW Welded Joints on Mechanical Properties of AA7075-T6 Aluminium Alloy
M. Sivashanmugama , M. A Essam Ahamed b ,Amithkishore Pc ,Venu Gopal Sd
aAssociate, Professor. Department of Mechanical & Production Engineering, Sathyabama University, Chennai,India.
bUG Student, Department of Mechanical & Production Engineering, Sathyabama University, Chennai, India
c Asst. Professor, Department of Mechanical Engineering, Sathyabama University, Chennai, India.
d Asst. Professor, Department of Mechanical Engineering, CK College of Engineering and Technology, Cuddalore 607 703, India.
Abstract- Friction stir, welding is a solid state joining process and is widely being considered for aluminium alloys. The main advantage of FSW is the material that is being welded undergoes only localized changes. The welding parameter and tool pin profile play a major role in deciding the weld quality. In this work an effort has been made to analyze microstructure of aluminium AA 7075-T6 alloy. Three different tool profiles (Taper Threaded, cylindrical and square) have been used to construct the joints in particular rotational speed. Tensile, Impact, micro hardness of mechanical properties of the joints have been evaluated and the formation of FSP zone has been analyzed microscopically. From the investigation it is found that the threaded cylindrical profile produces highly (defined) Strength in welds.
Keywords: AA 7075-T6 aluminium alloy; Friction stir welding; Tool pin profile; FSP zone; Tensile, Impact evaluation.
-
INTRODUCTION
AA7075-T6 is the most widely used material for the construction of leading and trailing edges, Helicopter rotor blades and navy bulk head joiner panels. It has unique combination of properties such as good weld ability, light weight and high strength properties. The normality used welding process properties. The normally used welding process for these materials is TIG, MIG, the electron beam welding process [1]. AA7075-T6 is a heat treatable alloy so for welding the rotational speed is considered for effective welding and the parameters are designed accordingly [2].
So, in considering the need of friction stir welding in vast application, the material is welded using friction application, the material is welded using friction stir welding process. Friction stir Welding (FSW) process is an emerging joining Technology than can eliminate usual defects that occur in the weld area and refine the microstructures, thereby improving strength and ductility, increasing resistance to corrosion and fatigue and enhance the properties of the weld.
(a)
(b)
Fig. 2- (a) An FSW weld between aluminum sheets. (b) An actual tool, with a threaded-pin
(c)
Fig. 3-Different regions of FSW joint: (a) unaffected base metal; (b) heat affected zone (HAZ); (c) thermo-mechanically affected zone (TMAZ); (d) friction stir processed (FSP) zone.
The FSW is usually carried out in solid an is a continuous hot shear autogenous weld involving a non consumable rotating probe of harder material than the material that abutting faces of the joint. The relative motion between the tool and base metals creates frictional heat by forming a plasticized zone near and around the tool. The tool shoulder also helps in containing the plasticized material in the weld region. As the tool traverses forward the plasticized material follows to form solid phase joint. The major advantage of FSW is that it follows local thermo mechanical metal working process without influencing properties of surrounding areas as observed in other welding process [3].
FSW joints consist of four different rejoins, they are (a)untouched base material (b)heat affected zone(HAZ) (c)Thermo mechanically heat affected zone(TMAZ) (d) Friction stir processing zone(FSP). These zones are normally affected by the rotating probe of the tool when it traverses the joint area. So probe to find relationship between tool profile and
Fig 4 .Square pin profile
Fig 5.Taper threaded pin profile
-
EXPERIMENTAL PROCEDURE:
The base metal used for the is Al-Zn alloy in which the manganese increases the corrosion resistance, ductility and toughness. The aluminum plates are cut into required size of (200mmX75mm) by power saw cutting and grinding. A single pass weld was made in the butt joint area. Butt joints have been made. The tool that was used is a non-consumable tool of made of high speed steel. Three different tools as shown in fig 2a&2b are made. Using each tool a single joint is made. The machine used for welding was specially made. The welding speed of 800rpm with table feed of 65mm/min was taken in consideration [4]. The load applied was 1 ton to achieve better weld without defects. The tool hardness was set between 50 to 70 HRC. Tool profile shapes and dimensions are shown in fig. 2a & 2b.
Fig 6. FSW Weldments
-
TEST
The welded joints are sliced through power hacksaw and machined to the required dimension to prepare tensile test specimens are shown in fig. 1b. American society for testing of materials (ASTME8-4) guidelines is followed for preparing the test specimens. Tensile test are carried out in the universal testing machine with reference to ASME- sec ix. Initially the was loaded 100KN, and then it is loaded gradually at the rate of 1.5KN/mm as per specification. The specimen fails after necking and load versus displacement has been recorded. The 0.2% offset yield strength; ultimate tensile strength and percentage of elongation have been evaluated. Micro hardness
test has been employed (Vickers hardness)[5] for measuring micro hardness across the joint with 0.2kg load.
Similarly the welded joints are sliced through power hacksaw and machined to required dimension to prepare specimen for tensile and impact test as shown in fig. American society for testing of materials guidelines is followed for preparing the test specimens. Tensile and impact tests are conducted in the respective machines. The values are recorded. The specimens for me.[8]
Fig.7.Schematic diagram of (a) tensile and (b) Impact specimen
Fig.8 Base metal AA7075 microstructure investigation
(Table- 1)
TABLE.1. BASE METAL AA7075 CHEMICAL COMPOSITION
-
RESULTS AND DISCUSSION
-
Tensile strength value
(Table- 2)
SL. NO
SAMPLE ID
UTS VALUE (N-m)
% ELONGATION
1
WST11
197.8
11
2
WST12
191.35
11.5
3
WST13
331.36
11.5
4
WST21
321.79
12
5
WST22
229.5
11
6
WST23
264.8
11
-
IMPACT VALUE
(Table- 3)
SL.N O
SAMPLE ID
AMBIENT TEMP (300C)
IMPACT VALUE(J)
1
WST11
300C
4
2
WST12
300C
4
3
WST13
300C
5
4
WST21
300C
4
5
WST22
300C
4
6
WST23
300C
6
Fig. 7.Tensile test specimens of Friction Stir Welded joints of A7075 before testing.
Figure .8 Tensile test specimens of Friction Stir Welded joints of AA7075 after.
Strength of
Threaded Pin in MPa
7 9 11
Axial Load(k
0
Effect of Axial Load on Tensile
Strength for both Profiles
500
Tensile
Tensile
Strength(MPa)
(a)
Effect of Axial Load on Tensile
Strength for both Profiles
500
0
7 8 9 10 11 12
Axial Load(k
Tensile
Strength of Threaded Pin in MPa
Tensile
Strength(MPa)
(b)
Effect of Axial Load on Impact
Impact Strength(Joule)
10 Strength for both profiles
Figure. 9 Impact Specimens before Testing for Friction Stir Welded joints
5
0
7 8 9 10 11 12
Axial Load(kN)
(c)
Impact Strength of Threaded Pin in Joule
Effect of Axial Load on Impact Strength for both profiles
Figure.10 Impact Specimen after Testing for Friction Stir Welded joints
-
Micro Hardness
10
Impact
ength(Joule)
7 8 9 10 11 12
Axial Load(kN)
(d)
Impact Strength of Threaded Pin in Joule
The micro hardness values for three different zones namely FSP, HAZ, Base mental is found.
Fig.11 (a) and (b) Effect of axial load on Tensile Strength for both profile; (c) and (d) Effect of axial load for Impact Strength for both Profile.[7]
The micro hardness test was performed using micro hardness machine for the square pin and taper threaded pin values are tabulated
SQUARE PIN PROFILE MICRO HARDNESS VALUE TABULATED:- TABLE 5
Weld
142
141
142
HAZ
142
141
142
TAPER THREADED PIN PROFILE MICRO HARDNESS VALUE TABULATED:- TABLE 6
Weld
182
180
176
HAZ
162
164
158
SAMPLE
PARAMETERS
BASE METAL
HAZ
WELD
SAMPLE
1 Taper Threaded
Pin
RST11- 1600 RPM, 8KN
182
172
165
SAMPLE2
Taper Threaded
Pin
RST21- 8KN,
75mm/min, 1500RPM
182
168
163
SAMPLE 3
Square Pin
RST21, 7 KN,
75mm/min, 1500RPM
182
155
152
SAMPLE
4 Square Pin
RST22, 9KN,
75mm/min, 1500RPM
182
161
162
T1-TAPER THREAD, 8KN, 75MM/MIN TABLE 7
-
Micro structure
Figure.13 Micro structure of TMT and weld zone
Shows the TMT zone where the direction of the base metal has changed due to the friction stir force and heat. The heat made the dissolved phase re-appear as bigger particles.[6]
Figure.14 Micro structure of weld zone
Shows the interface location of the TMT and weld zone. The particles in the weld zone are finer due to the fragmentation and growth.
The complete cross-section of the FSW zone with the parent metal on both the sides. The FSW zone shows the presence of unfilled tunnel cavity with the presence of some black particles.
Figure.12 Micro structure of Parent metal
Shows the parent metal microstructures which seem to be wrought aluminum alloy. The phases present are the Mg2Si and fine particles of Cu-al2. The matrix also shows the undissolved Al6 (Fe, Mn) inter metallics. The rolling bands along the direction of the rolling of the plate.
-
-
CONCLUSION
Considerable grain refinement has been achieved due to friction stir welding and the plastic flow. Due to retracting and advanced force the grains size are formed dynamic recrystallized zone
The Taper threaded cylindrical pin profile has been best suited at 800 rpm for better tensile strength, HAZ 172,168 and in weld zone 165,163 weld results and higher quality for this alloy.
The results can be applied for replacement of rivets in aircraft, rocket propulsion and automobile sectors where this alloy is used.
REFERENCES
-
Elangovan,V Balasubramanian Influence of tool pin profile and welding speed on the formation of friction stir processing zone in AA2219 alloy
-
K. Elangovan,V Balasubramanian Influence of tool pin profile and rotational speed of the tool by (journal)
-
yutaka A sato,Yusuke Sugiura, park,kokwa,Ikeda Post welded formability of friction stir welded aluminium alloy 5052
-
A. Scialpi,L.A.C De Filippies,P.Caviliere Influence of shoulder geometry on microstructure and mechanical properties of friction stir welded 6082 aluminium alloy
-
Thomas, W.M.; et al.: friction stir welding, U.S.Patent 5,460,317.
-
Dawes, C.J.; and Thomas, W.M.:Friction Stir Process Welds Aluminium Alloys, Welding Journal, pp.41 45, March 1996.
-
Midling, O.T.;Material Flow Behaviour & Microstructural Integrity of Friction Stir Butt Weldments, Fourth International Conference. In Aluminium alloys, pp. 451 458, September 1994.
-