Microstructure, Wear and Corrosion Characteristics of 304 Stainless Steel Laser Cladded with Titanium Carbide

DOI : 10.17577/IJERTV4IS080457

Download Full-Text PDF Cite this Publication

Text Only Version

Microstructure, Wear and Corrosion Characteristics of 304 Stainless Steel Laser Cladded with Titanium Carbide

Essam R. I. Mahmoud

Welding and NDT Lab., Manufacturing Technology Department Central Metallurgical Research and Development Institute (CMRDI) Cairo, Egypt.

Abstract Aiming to increase the wear resistance of 304 stainless steel alloy without significant losses in its corrosion resistance, it was YAG fiber laser cladded with TiC powder at fixed processing power of 2800 W and travelling speeds of 4, 8, and 12 mm/s. The TiC powder with a particle size of 3-10 m were preplaced on the cleaned surface to form a layer of two different thicknesses; 1 and 2 mm. Argon gas was used as a shielding during and after laser cladding at flow rate of 15 L/min. Some of the TiC particles were melted and re-solidified as dendrites during the cladding processing. The amount of the dendritic TiC structure was increased by increasing of the travelling speed. The cohesion of the cladding layer with the substrate was improved with increasing the travelling speed. At lower travelling speed, cracks were appeared at both the interface and the heat affected zone. The TiC particles were clustered in the top portion of the cladding layer when the preplaced powder was 2 mm. The surface hardness and wear resistance were remarkably improved at all processing conditions, especially at higher travelling speeds. Moreover, the sample treated at travelling speed of 12 mm/s showed better corrosion resistance than the stainless steel substrate.

Keywords Laser cladding; 304 stainless steel alloy; TiC powder; Surface microhardness; Wear and Corrosion resistance.

  1. INTRODUCTION

    AISI 304 stainless steel alloy is widely used in various fields, such as oil, nuclear and chemical industries due to its specific properties, i.e. excellent corrosion resistance, good mechanical properties and accepted machinability [1-2]. This type of stainless steels is used as a structural material in hydraulic machinery and in liquid-handling systems [3-4]. However, at severe environments, where the wear and cavitation attack are the main failure modes, this type of steel cannot be used due to its low surface hardness and wear resistance. Due to the contact between the components and a flowing or vibrating liquid, cavitation erosion represents a common type of degradation of components [5]. Generally, good wear, corrosion and oxidation resistances of different materials can be obtained by tailoring their surface properties. This can be done by depositing some alloys and/or ceramic powders on the material surfaces aiming to produce metal matrix composites

    (MMCs) on the treated surfaces. This can be produced by laser cladding. The advantages of this technique over the conventional ones (such as arc welding and thermal spraying) include: better coatings with dense microstructure, high wear resistance, low dilution and good metallurgical bonding to substrate [6-8]. Different substrate materials such as steels, aluminum [9-10] and titanium alloys [11-12] were cladded by this treatment. Ceramic powders such as SiC [6] , TiC [11-12] and WC [13] without/or with some materials such as Ni-based alloy [14] were added as cladding materials. TiC has many excellent advantages, such as very high melting point and thermal stability, high hardness and excellent wear resistance, low coefficient of friction, good resistance to thermal shock, high electrical and thermal conductivities and is widely used as the reinforcement in many wear resistant materials [15-17]. Moreover, the TiC particles have good compatibility with the iron base matrix [18].

    Some works have been done to clad the stainless steel alloys with ceramic powder by using laser technique aiming to improve the wear and cavitation erosion resistances [19]. However, the increase in cavitation erosion resistance was usually accompanied by some degree of deterioration in corrosion resistance [19]. In these studies, the increase in cavitation erosion resistance is mainly attributable to an increase of hardness arising from the presence of hard phases. But the presence of these phases deteriorates the passive film. In other studies, the surface hardening of austenitic stainless steel has been achieved by incorporating the hard particles of TiC, SiC, WC and alloying elements [20] in order to form carbides, nitrides [21] and borides [22]. In other studies, element such as Mo [23] was added to improve the pitting and intergranular corrosion resistance and to prevent stress corrosion cracking in acoustic environment. To widen the applications of 304 stainless steel alloy, it is important to improve its wear resistance without losses in its corrosion resistance. In the present study, 304 stainless steel substrate is laser cladded with TiC powder using YAG fiber laser. The effect of travelling speed and the thickness of the preplaced powder on the microstructural features, hardness, wear and corrosion resistance will be studied.

  2. EXPERIMENTAL WORK

    Stainless steel (304) specimens with dimensions of 100 mm x 50 mm x 3 mm were used as substrate materials. The specimens were ground using emery papers and cleaned in acetone to remove any dirt, oil, grease and other contaminants before treatment. The TiC powder with a particle size of 3-10 m were preplaced on the cleaned surface to form a layer of two different thicknesses; 1 and 2 mm. The cladding treatments were carried out using YAG fiber laser of 3 kW. To avoid the oxidation during the treatment, argon gas with the flow rate of 15 l/min was used as a shielding gas. The treatments were carried out at fixed processing power of 2800 W, which was considered the optimum power during the preliminary experiments. Three different travelling speeds of 4, 8 and 12 mm/s were used in this study. The process was conducted at a defocusing distance (Df) of 65 mm. The microstructures of the coated layer and substrates were investigated using optical microscope and scanning electron microscope equipped with EDX analyzer. The micro-Vickers hardness in the coated layer cross-section and the substrate were measured with an indentation load of 9.8 N and loading time of 15s at room temperature. The wear behaviour of the laser cladded zone was evaluated using a pin-on-disk dry sliding wear tester in air at room temperatures. A stationary sample with a diameter of 2.5 mm was slid against a rotating disk with a rotational speed of 265 rpm for 15 min. The tests were carried out at a fixed load of 2 kg applied to the pin. Before the test, all the specimens were ground on emery paper up to # 600 to get smooth and flattened surface. The specimens were weighted before and after the test with a sensitive electronic balance with an accuracy of 0.001 g. The differences in average weight before and after the wear test were measured and accounted. Three specimens of each condition were chosen for wear tests. The untreated base metal was selected as the reference material for the wear test. The corrosion behavior of the substrate and the cladding layer were evaluated by the corrosion current density and the corrosion potential obtained from polarization curves in a 3.5 wt.% NaCl solution at room temperature with an IM-6 electrochemical workstation. The scanning potential can be in the range of -1.0 to +2 V, and the scanning rate was 5 mV/s.

  3. RESULTS AND DISCUSSION

    1. Microstructure analysis

      The basic microstructure of the substrate, as shown in Fig. 1, is constituted of equiaxed, twinned austenitic-grain structure, which is the typical microstructure of the 304 austenitic stainless steel alloy. Macro-view of the cros-section of the cladding layer synthesized with laser power and travelling speed of 2800 W and 12 mm/s, respectively is shown in Fig. 2. The cladding zone appeared as a concaved shape inside the substrate. This is may be due to the large defocusing distance (65 mm), which focus the heat into deeper areas. From this figure, the cross-section of the laser treated area was composed of TiC rich zone, heat affected zone and the substrate.

      Figures 3 and 4 show the microstructures of the cladded layer fabricated with preplaced TiC powder of 1 mm thick and 4 mm/s travelling speed. Most of the TiC powder were dissolute in the matrix, forming fine dendrites with small arms as shown in Fig. 3 (a and b).

      Fig. 1 Microstructure of the 304 stainless steel substrate.

      Fig. 2 Macrograph of the laser treated zone at power of 2800 W and travelling speed of 12 mm/s.

      Fig. 3 Micrographs of the different zone at laser treated layer with power of 2800 W and travelling speed of 4 mm/s, when the thickness of preplaced TiC power was 1 mm, where (a) and (b) at the cladding layer, and (c) and ((d) at the interface.

      At the lower portion of the cladding layer, many cracks and crack networks were observed which starts from the interface and going upward into the cladding layer as shown in Fig. 3 (c and d). This is may be due to the lower thermal conductivity of the stainless steel substrate, which may result in keeping of higher temperature for a longer time and reducing the cooling rate, and leads to formation of carbides at the grain boundary of the stainless steel side. This explanation was confirmed with the micrographs shown in Fig. 4. The treated specimen with this slow travelling speed (4 mm/s) had a wide heat affected zone (Fig. 4 (a)) and their grain boundaries were attacked (Fig. 4 (b)) due to the formation of carbides at the grain boundaries.

      Fig. 4 Micrographs of the heat affected zone of the specimen treated with power of 2800 W and travelling speed of 4 mm/s, when the thickness of preplaced TiC power was 1 mm.

      Fig. 5 Micrographs of the different zone at laser treated layer with power of 2800 W and travelling speed of 8 mm/s, when the thickness of preplaced TiC power was 1 mm, where (a) and (c) at the interface, and (b) and ((d) at the cladding layer.

      When the travelling speed was increased twice to be 8 mm/s, no micro-cracks were observed in the cladding layer or at the interface as shown in Fig. 5. The cladding layer looks adhered to the substrate and free from the macro-defects. The TiC particles were partially dissolute and appeared as fine long dendrites together with their original shape, especially at the top portion (near the free surface). At the lower portion (near the substrate), the TiC dendrites were shorter and they had random orientation (Fig. 5 (b)). This is mainly due to the lower heat dissipation to the lower thermal conductivity stainless steel substrate. Moreover, some pores were detected in the cladding layer.

      By increasing the travelling speed to 12 mm/s, the interface between the cladding layer and the substrate stainless steel is adherent, sharp and defect free as shown in Fig 6. The TiC in the cladding layer was distributed homogenously and consisted of fine long dendrites at the top portion and at the lower contour of the cladding layer. This may be due to the relatively fast cooling rate after faster travelling speed. In some areas at the center of the cladding layer, some of the TiC particles appeared as short random oriented dendrites. Moreover, some of these carbides appeared as a rosette shape morphology as shown in Fig. 7.

      Fig. 6 Micrographs of the different zone at laser treated layer with power of 2800 W and travelling speed of 12 mm/s, when the thickness of preplaced TiC power was 1 mm.

      Fig. 7 Micrographs (a – c)of the cladding layer with power of 2800 W and travelling speed of 12 mm/s, when the thickness of preplaced TiC power was 1 mm, and (d) EDX spectra of the elements of red mark in (c).

      In severe applications, where the wear is a main failure mode, it is better to increase the thickness of the hard layer deposited on the substrate. For this reason, the thickness of the preplaced TiC powder was increased to be 2 mm. The used processing power and travelling speed were 2800 W and 4 mm/s, respectively. The produced cross-section microstructures were shown in Fig. 8. The cladding layer was consisted of two regions. The TiC powder appeared as dense clusters of interlocked particles in the upper portion. At these areas, there was almost no stainless steel matrix as shown in Fig. 8 (b). The lower portion of the cladding layer was composed of TiC particles with their round shape surrounded by the stainless steel matrix. The heat generated is not enough to melt the thick TiC particles layer. Near the interface, some TiC particles were melted and appeared as dendrites with random orientation or rosette shape as shown in Fig. 9.

      Fig. 8 Micrographs of the different zone at laser treated layer with power of 2800 W and travelling speed of 4 mm/s, when the thickness of preplaced TiC power was 2 mm, where (a) and (d) at the interface, (b) at the top portion of the cladding layer, and ((c) at the lower portion of the cladding layer.

      Fig. 9 Micrographs of the cladding layer with power of 2800 W and travelling speed of 4 mm/s, when the thickness of preplaced TiC power was 2 mm.

    2. Surface and subsurface microhardness evaluation

      Headings, Figure 10 shows the microhardness distribution through the depth of the laser treated zone obtained at different travelling speeds (4, 8, 12 mm/s) and preplaced powder thicknesses (1 and 2 mm). Generally, the hardness of the cladding layer is much higher (almost three times) than that of the base metal. This is may be due to the hard TiC particles which were distributed homogenously through the cladding layer. The cladding layer which formed with faster travelling speeds show higher hardness that that formed with slower ones. This is due to that the faster travelling speeds yields a finer dendritic TiC, which share in hardness increment. The average hardness values at the surface treated by 12 mm/s travelling speed was about 600 HV.

      When the preplaced TiC powder thickness was increased to 2 mm thick, the cladding layer showed ultra-high hardness values (reached to more than 2000 HV), especially at the top portion of the cladding layer (near the free surface). This is due to the compacted dense hard TiC particles that formed on the top portion of the cladding layer.

      Fig. 10 Microhardness distributions through the laser treated layer cross- sections at different travelling speeds and preplaced powder thicknesses, and fixed power of 2800 W.

    3. Wear and corrosion resistance of the developed surface layer

      Figure 11 shows the variation of wear weight losses of the laser cladding layers using different laser travelling speeds (4, 8, 12 mm/s) and preplaced powder thicknesses (1 and 2 mm) together with the substrate, after subjected to pin-on-disk dry sliding wear test at a fixed load of 2 kg in air at room temperatures. Compared with the substrate, the wear resistance of the laser cladding layer was improved by at least three times. The wear rate was decreased by increasing the travelling speed. This is may be due to the higher hardness achieved at these speeds. On the other hand, the sample that had a preplaced TiC powder of 2 mm, showed exceptional wear resistance (the wear rate was very small, about 0.02 gm). This improvement in wear resistance came from the hard, wear resistant, and dense TiC particles which formed at this condition.

      Regarding the corrosion resistance evaluation, the sample cladded at travelling speed of 12 mm/s and processing power of 2800 W was chosen due to that it gave the best results regarding the microstructure, hardness and wear resistance. Fig.12 shows the polarization curves of stainless steel substrate and the cladding layer. From this figure, it is clear that the corrosion potential of the cladded sample was shifted to more positive than that of the stainless steel substrate. Also, the corrosion current of the cladded layer showed lower values than that of the stainless steel substrate. It is well known that when the potential is increased and the current is decreased, the polarization resistance is increased and the material show improved corrosion resistance. Thus, it is clearly evident that the laser cladding of TiC particles on the stainless steel substrate had a positive influence on the corrosion behavior of the coatings. This can be related to the finer microstructure obtained in this cladding layer and to the good metallurgical bonds of the TiC particles/dendrites with the matrix which give higher chemical stability of the coating.

      Fig. 11 Wear weight losses of the substrate and specimens treated at different travelling speeds (4, 8, 12 mm/s) and preplaced powder thicknesses

      (1 and 2 mm), and fixed power of 2800 W.

      Fig. 12 Polarization curves of the substrate (a), and the cladding layer produced with travelling speed of 12 mm/s and processing power of 2800 W.

  4. CONCLUSIONS

304 stainless steel specimens were YAG fiber laser cladded with TiC powder using processing power of 2800 W and travelling speeds of 4, 8 and 12 mm/s. The TiC powder with a particle size of 3-10 m were preplaced on the cleaned surface to form a layer of two different thicknesses; 1 and 2 mm. The microstructures of the coated layers and substrate were investigated. The micro-Vickers hardness was measured through the depth of the coated layers cross-section. The wear behaviour of the laser cladded layers was evaluated. The

corrosion behavior of the substrate and the cladding layer were evaluated by the corrosion current density and the corrosion potential obtained from polarization curves in a 3.5 wt.% NaCl solution at room temperature. The results of this study lead to the following conclusions:

    1. Metal matrix composite reinforced with TiC particles was produced in the cladded layer on 304 stainless steel specimens by application of laser cladding treatment at all processing conditions.

    2. Some of the TiC particles were melted and re-solidified as dendrites during the cladding processing. The amount of the dendritic TiC structure was increased by increasing of the travelling speed.

    3. The cladding layer produced with higher travelling speed (12 mm/s) was tightly bonded with the substrate without any cracks or any other defects, while that produced at travelling speed of 4 mm/s showed some cracks and crack-networked at the interface and the heat affected zone.

    4. The TiC particles were clustered in the top portion of the cladding layer when the preplaced powder was 2 mm.

    5. The hardness of the cladding layer was improved at all processing conditions to be three times at 12 mm/s travelling speed. When the preplaced TiC power was increased to 2 mm, the hardness showed ultra-high values (more than 2000 HV).

    6. The wear resistance of the cladding layers was remarkably improved especially at higher travelling speed.

    7. The corrosion resistance of the cladding layer produced by travelling speed of 12 mm/s was better than that of the stainless steel substrate.

REFERENCES

  1. Anwar U.H., Hani M.T., and Nureddin M. A., Failure of weld joints between carbon steel pipe and 304 stainless steel elbows, Engineering Failure Analysis, Vol. 12, pp. 181191, 2012.

  2. Fissoloa A., Stelmaszykb J. M., Gourdin C., Bouin P., and Pérez G., Thermal fatigue loading for a type 304-L stainless steel used for pressure water reactor: investigations on the effect of a nearly perfect biaxial loading, and on the cumulative fatigue life, Procedia Engineering, Vol. 2, pp. 1595604, 2010.

  3. Chiu K.Y., Cheng F.T., and Man H.C., Laser cladding of austenitic stainless steel using NiTi strips for resisting cavitation erosion, Materials Science and Engineering: A, Vol. 402, pp. 126134, 2005.

  4. Majumdar J. D., Ramesh B. Chandra, and Manna I., Laser composite surfacing of AISI 304 stainless steel with titanium boride for improved wear resistance, Tribology International, Vol. 40, pp. 146152, 2007.

  5. Li S.C. , Cavitation damage in turbines, in: S.C. Li (Ed.), Cavitation of Hydraulic Machinery, Imperial College Press. pp. 277294, 2000.

  6. Yang Y.L., Guo N., and Li J.F., Synthesizing, microstructure and microhardness distribution of TiSiCN/TiCN composite coating on Ti6Al4V by laser cladding, Surface and Coatings Technology, Vol. 219, pp. 17, 2013.

  7. Qiu X.W., Zhang Y.P., He L., and Liu C.G., Microstructure and corrosion resistance of AlCrFeCuCo high entropy alloy, Journal of Alloys and Compounds, Vol. 549, pp. 195199, 2013.

  8. Guo C., Zhou J.S., Chen J.M., Zhao J.R., Yu Y.J., and Zhou H.D., Improvement of the oxidation and wear resistance of pure Ti by laser cladding at elevated temperature, Surface and Coatings Technology, Vol. 205, pp. 21422151, 2010.

  9. Thawari G., Sundarararjan G., and Joshi S.V., Laser surface alloying of medium carbon steel with SiC(P), Thin Solid Films, Vol. 423 (1), pp. 4153, 2003.

  10. Liang G.Y., T.T. Wong, J.M.K. MacAlpine, and J.Y. Su. , Study of wear resistance of plasma-sprayed and laser-remelted coatings on aluminium alloy, Surface and Coatings Technology, Vol. 127, pp. 233238. 2000.

  11. Sun R.L., Yang D.Z., Guo L.X. (2001). Laser cladding of Ti6Al4V alloy with TiC and TiC+ NiCrBSi powders, Surface and Coatings Technology, Vol. 135, 307312, 2001.

  12. Sun R.L., Mao J.F., and Yang D.Z., Microscopic morphology and distribution of TiC phase in laser clad NiCrBSiCTiC layer on titanium alloy substrate, Surface and Coatings Technology, Vol. 155 (23), pp. 203207, 2002.

  13. Mateos J., Cuetos J.M., Fernandez E., and Vijande R., Tribological behavior of plasma-sprayed WC coatings with and without laser remelting, Wear, Vol. 239, pp. 274281, 2000.

  14. Cheng F.T., Kwok C.T., and Man H.C., Laser surfacing of S31603 stainless steel with engineering ceramics for cavitation erosion resistance, Surface and Coatings Technology, Vol. 139 (1), pp. 1424, 2001.

  15. Liu Y.F., Mu J.S., Xu X.Y., and Yang S.Z. , Microstructure and dry- sliding wear properties of TiC-reinforced composite coating prepared by plasma-transferred arc weld-surfacing process, Materials Science and Engineering: A, Vol. 458, pp.366370, 2007.

  16. Dong Y.J., and Wang H.M., Microstructure and dry sliding wear resistance of laser clad TiC reinforced TiNiSi intermetallic composite

    coating, Surface and Coatings Technology, Vol. 204, pp. 731735, 2009.

  17. Deng J., Liu L., Yang X., Liu J., Sun J., and Zhao J., Self-lubrication of Al2O3/TiC/CaF2 ceramic composites in sliding wear tests and in machining processes, Materials and Design, Vol. 28, pp. 757764, 2007.

  18. Jose´ S. M., Sonia Lopez-Esteban, and Carlos P., The challenge of ceramic/metal microcomposites and nanocomposites, Progress in Materials Science, Vol. 52, pp.10171090, 2007.

  19. Lo K.H., Cheng F.T., and Man H.C., Cavitation erosion mechanism of S31600 stainless steel laser surface-modified with unclad WC, Materials Science and Engineering: A, Vol. 357, pp.168180, 2003.

  20. Laroudie F., Tassin C., and Pons M., Hardening of 316L stainless steel by laser surface alloying, Journal of Materials Science, Vol. 30, pp. 3652-3657, 1995.

  21. Viswanathana A., Sastikumar D., Rajarajan P., Kumar H., and Nath A.K., Laser irradiation of AISI 316L stainless steel coated with Si3N4 and Ti, Optics and Laser Technology, Vol. 39, pp.1504-1513, 2007.

  22. Zhang D., and Zhang X., Laser cladding of stainless steel with Ni- Cr3C2 and Ni-WC for improving erosive-corrosive wear performance, Surface and Coatings Technology, Vol. 190, pp. 212-217, 2005.

  23. MajumdarJ. D., and Manna I., Laser surface alloying of AISI304- stainless steel with molybdenum for improvement in pitting and erosioncorrosion resistance, Materials Science and Engineering: A, Vol. 267, pp. 50-59, 1999.

Leave a Reply