The Combined Influence of Polypropylene Fibers[PPF] and Silica Fume[SF]on Concrete Strength

DOI : 10.17577/IJERTV6IS080039

Download Full-Text PDF Cite this Publication

Text Only Version

The Combined Influence of Polypropylene Fibers[PPF] and Silica Fume[SF]on Concrete Strength

K.I.M. Ibrahim

Construction Engineering Dept., College of Engineering at Qunfudha , Umm-Al-Qura University- KSA on Sabbatical leave from higher Institute of Engineering and Technology of Kafr-EL-shiekh Egypt

Abstract:- This research investigates The combined Influence of PPF and SF on Concrete Strength. key variables Effects such as contents of PPF and SF were studied. An experimental plan was conducted to achieve the required objectives. Concrete mixes having a fixed water/binder ratio

available for commercial use, the main types being glass, steel ,synthetic materials, and some natural fibers [6-10]. Because PPF has low elastic modulus, high strength, low price, excellent ductility, and excellent durability, many of experimental works related to the PPF using in concrete

equals

    1. and a constant

      total binder content equals

      and cement matrix have been published.[11-12] The

      500kg/m3are prepared. The % of SF that replaced cement in this study were 0%,6%,12% and 18%. PPF with 12mm length and four volume fractions of 0%, 0.25%,0.5% and 0.75% are used. The results illustrate that SF posses great enhance on the concrete tensile and compressive strengths. The increasing of replacement of SF from 12% to 18% has no approximately significant change on the development of concrete strength. The adding of PPF caused an inverse influence on the strengths of plain and SF concretes.

      Keywords: Polypropylene Fibers[PPF] ,Compressive Strength And Silica Fume[SF]

      1. INTRODUCTION

        SF consists of extremely fine particles approximately 100 times lower than the average particles of cement, the great fineness of particles of the SF allows it to fill the tiny voids between cement particles . SF is among one of the important pozzolanic materials presently used in concrete. It was initial used in 1969 in Norway but only began to be systematically employed in Europe and North America in 1980. Since then, the SF using in concrete has been growing rapidly , it has been used either as a cement partial replacement or as an additive when special properties are desired [1]. The quick growth in the SF using is attributed to its positive effects on the cementitious composites mechanical properties . Trough the last decade considerable attention has been given to the SF using as a cement partial replacement to produce high-strength concrete[HSC]. the adding of SF to cement concrete marginally decreased the concrete workability but significantly enhanced its mechanical properties[2] . Bhanja et al. checked the SF influence on concrete and suggested the optimum SF content with view of the concrete compressive strength [3]. However, many of researches show that SF growths the concrete brittleness. Ductility improvement is a main aim in concrete science and must be taken into consideration by researchers [4,5] . For several centuries fibers have been used to reinforced brittle materials such as masonry bricks . Now, there are a many of fiber types

        polypropylene fibers effect on the hardened concrete properties changes depending upon the fiber length , fiber volume fraction , the design of mixture, and the concrete materials used nature . The common results indicate to abrasion resistance, permeability, and impact resistance are all considerably enhanced by the PPF addition [13] The PPF effect on compressive ,flexural, and tensile strengths in addition to toughness and Young modulus is not quite obvious. Most researches show either no effect or modest enhance in these properties. However, in some cases the PPF addition has been decreased the hardened concrete ultimate strength . The PPF using combined with SF can be recommended to decrease early age cracks and enhancing the durability. The combination of 0.07% PPF and 10%SF volumetric fraction mitigated early age cracks and much decrease carbonation depth and water permeability [14]. However, little information is presently recognized regarding to the combined effect of SF and PPF on the concrete mechanical properties . Therefore, the present study investigates SF, and PPF using an wide range of mixes : SF (by mass) from 6% to 18 % , and PPF (by volume) from 0.25% to 0.75% .

      2. MATERIALS

        in all concrete mixes, Local materials were tested and used according to ASTM [American Standard of Testing Materials] and ESS [Egyptian Standard Specifications]to in this study . basalt with maximum size equals to 25mm was used as a coarse aggregate and its particle shape was approximately flaky, in this research, natural sand composed essentially of siliceous materials was used as a fine aggregate .Ordinary Cement was checked to assure its compliance with Specifications . supper-plasticizer was added to maintain the water/ binder ratio =0.40 with slump ranges from 6-11cm. 12mm length PPF was used. For preparing the SF concretes , silica fume from Sika company was used.

      3. CONCRETE MIXES PROPORTIONS

        16 concrete mixes were prepared, and the initial one was without SF and PPF[ control mix]. There are 3 ratios of PPF by volume [ 0.25% ,0.5% , 0.75% ] were mixed in concrete and 3 ratios with SF by mass [6% , 12% , 18% ]

        replacing the similar quantity of cement. Another 9 proportions were arranged with SF by mass replacing the similar quantity of cement [6% to 18% ]with PPF mixed in concrete by volume [0.25% to 0.75%] . 16 mixes are shown in Table (1) .

        Table (1) : Concrete Mixes

        Mix No.

        PPF

        content

        %

        SF content

        Cement (kg/m3)

        Basalt kg/m3

        sand kg/m3

        water kg/m3

        Super plasticizer kg/m3

        %

        (kg/m3)

        1

        0

        0

        0

        500

        1130

        565

        200

        9.25

        2

        0.25

        0

        0

        500

        1130

        565

        200

        9.25

        3

        0.5

        0

        0

        500

        1130

        565

        200

        9.5

        4

        0.75

        0

        0

        500

        1130

        565

        200

        9.5

        5

        0

        6

        30

        470

        1130

        565

        200

        9.25

        6

        0

        12

        60

        440

        1130

        565

        200

        9.5

        7

        0

        18

        90

        410

        1130

        565

        200

        9.5

        8

        0.25

        6

        30

        470

        1130

        565

        200

        9.5

        9

        0.5

        6

        30

        470

        1130

        565

        200

        10

        10

        0.75

        6

        30

        470

        1130

        565

        200

        /td>

        10

        11

        0.25

        12

        60

        440

        1130

        565

        200

        9.5

        12

        0.5

        12

        60

        440

        1130

        565

        200

        10

        13

        0.75

        12

        60

        440

        1130

        565

        200

        10

        14

        0.25

        18

        90

        410

        1130

        565

        200

        9.75

        15

        0.5

        18

        90

        410

        1130

        565

        200

        10

        16

        0.75

        18

        90

        410

        1130

        565

        200

        10

      4. DESCRIPTION OF TESTED SPECIMENS

        48 cubes of sides15x15x15cm length and 48 cylinders of diameter 15cm and height 30cm were cast for compressive and splitting tensile strengths .Concrete was cast and compacted in the forms. Hydraulic compression machine of 2000KN capacity was used for testing the specimens.

      5. TEST RESULTS COMPRESSIVE STRENGTH Concrete mixes compressive strengths were specified at 28 days of curing. The results are illustrated in Tables 2-7 and Figures 1-6. Table 2 and figure 1 show the change of polypropylene fiber reinforced concrete (PPFRC) compressive strengths. From this results, with increasing of PPF content, the compressive strength is reducing gradually and the reduction is so great at the PPF content equals 0.75%. Compared with plain concrete, the reduction of compressive strength was 20 % , 25 % and 26 % for PPF content equals 0.25% , 0.50% and 0.75% respectively. Table 3 and figure 2 show the change of compressive strength of silica fume concrete (SFC)mixes , from this results ,the compressive

        strength growths with increasing of SF contents and the different SF contents strengths are bigger than that of control mix. Compared with the control mix, the compressive strength increases of 13% , 45 % and 23 % for SF contents 6% , 12% and 18% respectively. SF acts as a filler because of its tiny particles size and the pozzolanic response of the SF produces extra C-S-H gel , which grows into the capillary spaces that remain after the cement hydration in mortar mixes [15]. Therefore , it would appear that SF acts both physically (as space filler) and chemically (reacting with Ca(OH)2 to form C-S-H) to aid in the improvement of mixes strength .

        Tables 4-6 and figures 3-5 show the change of the PPFRC compressive strength at the same ratios of SF contents. It was noticed that with increasing of PPF contents, the SFC compressive strength decreases. At 6% SF, the compressive strength reduces with 26%, 29% and 30% for

        PPF content equals to 0.25%, 0.5% and 0.75% respectively while at SF content 12% the decrease was 29% , 40% and 41%, also at 18% SF content the decrease

        was 22%, 32% and 34% respectively

        Table (2): Compressive strength results [kg/cm2] of PPFRC

        SF content %

        PPF content %

        Compressive strength kg/cm2

        0

        0

        [control]386

        0

        0.25

        [-20%]310

        0

        0.5

        [-25%]291

        0

        0.75

        [-26%]287

        450

        400

        350

        300

        250

        200

        150

        100

        50

        0

        0%ppf

        0.25%ppf

        0.5%ppf

        0.75%ppf

        fiber volume fraction

        compressive strength kg/cm2

        Fig.(1) : The PPFRC compressive strength (kg/cm2)

        [+23%]475

        18

        [+13%]436

        Compressive strength kg/cm2

        PPF content %

        compressive strength kg/cm2

        Table (3): Compressive strength results [kg/cm2] of SFC

        SF content %

        0

        0

        [control]386

        6

        0

        12

        0

        [+45%]560

        0

        600

        500

        400

        300

        200

        100

        0

        0%SF

        6%SF

        12%SF

        18%SF

        silica fume %

        Fig.(2) : The SFC compressive strength (kg/cm2)

        Table (4): PPFRC with SF content =6% compressive strength results [kg/cm2]

        SF content %

        PPF content %

        Compressive strength kg/cm2

        6

        0

        [control]436

        6

        0.25

        [-26%]324

        6

        0.5

        [-29%]308

        6

        0.75

        [-30%]304

        500

        450

        400

        350

        300

        250

        200

        150

        100

        50

        0

        0%ppf

        0.25%ppf

        0.5%ppf

        0.75%ppf

        fiber volume fraction

        compressive strength kg/cm2

        Fig.(3) : PPFRC with SF content =6% compressive strength results [kg/cm2]

        Table (5): PPFRC with SF content =12% compressive strength results

        [kg/cm2]

        SF content %

        PPF content %

        Compressive strength kg/cm2

        12

        0

        [control]560

        12

        0.25

        [-29%]400

        12

        0.5

        [-40%]338

        12

        0.75

        [-41%]328

        600

        500

        400

        300

        200

        100

        0

        0%ppf

        0.25%ppf

        0.5%ppf

        0.75%ppf

        fiber volume fraction

        compressive strength kg/cm2

        Fig.(4) : PPFRC with SF content =12% compressive strength results [kg/cm2]

        Table (6): PPFRC with SF content =18% compressive strength results [kg/cm2]

        SF content %

        PPF content %

        Compressive strength kg/cm2

        18

        0

        [control]475

        18

        0.25

        [-22%]370

        18

        0.5

        [-32%]322

        18

        0.75

        [-34%]315

        500

        450

        400

        350

        300

        250

        200

        150

        100

        50

        0

        0%ppf

        0.25%ppf

        0.5%ppf

        0.75%ppf

        fiber volume fraction

        [+10%]315

        [+14%]328

        [+6%]304

        [control]287

        0.75

        [+11%]322

        [+16%]338

        [+6%]308

        [control]291

        0.5

        [+19%]370

        [+29%]400

        [+5%]324

        [control]310

        0.25

        [+23%]475

        [+45%l]560

        [+13%l]436

        [control] 386

        0

        12%

        6%

        the compressive strength (kg/cm2) at SF content

        PPF content%

        400

        500

        compressive strength kg/cm2

        compressive strength kg/cm2

        Fig.(5) : PPFRC with SF content =18% compressive strength results [kg/cm2] Table (7): Summary of compressive strength results [kg/cm2]

        0%

        18%

        600

        0

        0%ppf

        0.25%ppf 0.5%ppf 0.75%ppf

        0%SF

        6%SF

        12%SF

        18%SF

        100

        300

        200

        Fig.(6) : The compressive strength (kg/cm2) of all concrete mixes

        Tensile strength

        Splitting tensile strengths of all mixes were specified after 28 days curing. The results are given in Tables 8-13 and Figures 7-

        12. Table 8 and figure 7 show the change of PPFRC tensile strength. From this results, with increasing of fiber content, the tensile strength is reducing regularly . Compared with plain concrete ,the decrease of tensile strength were 10 % , 18% and 16 % for 0.25% , 0.50% and 0.75% PPF content respectively. Table 9 and figure 8 show the change of SFC tensile strength , from these results ,the tensile strength growths with increasing of SF contents and the strengths of different SF contents are larger than that of control mix. Compared with the control mix, the tensile strength increases of about 11 % , 25 % and 22 % for SF

        contents 6% , 12% and 18% respectively. Tables 10-12 and figures 9-11 show the variation of the tensile strength of PPFRC at the same ratio of SF content. With increasing PPF content, the SFC tensile strength decreases. At 6% SF content ,the tensile strength decreases with 10%, 16% and 16% for PPF content 0.25%, 0.5% and 0.75% respectively as for SF content 12% the

        decrease was 18%,24% and 24%, also for SF content 18% was 20%, 28% and 23% respectively.

        tensile strength kg/cm2

        Table (8): PPFRC tensile strength results [kg/cm2]

        SF content %

        PPF content %

        Tensile strength kg/cm2

        0

        0

        [control]37

        0

        0.25

        [-10%]33

        0

        0.5

        [-18%]30

        0

        0.75

        [-16%]31

        40

        35

        30

        25

        20

        15

        10

        5

        0

        0%ppf

        0.25%ppf

        0.5%ppf

        0.75%ppf

        fiber volume fraction

        Fig.(7) : The PPFRC tensile strength (kg/cm2)

        Table (9): SFC tensile strength results [kg/cm2]

        SF content %

        PPF content %

        Tensile strength kg/cm2

        0

        0

        [control]37

        6

        0

        [+11%]41

        12

        0

        [+25%]46

        18

        0

        [+22%]45

      6. CONCLUSIONS

  1. SF has an inverse effect on the fiber concrete workability.

  2. SF has great enhance on the concrete compressive strength and concrete splitting tensile strength , the splitting tensile strength and compressive strength of concrete increase gradually with increasing the content of SF.

  3. The compressive strength increases with increasing in SF compared with normal concrete. The maximum increase in compressive strength was up to 13 %, 45 % and 23 % for 6% , 12% and 18% of SF replaced by cement respectively.

  4. The tensile strength increases with increasing in SF compared with normal concrete. The maximum increase in strength was 11 %, 25 % and 22 % for 6% , 12% and 18% of SF replaced by cement respectively.

  5. The increase of replacement levels of SF from 12% to 18% has not large change on the development of tensile and compressive strengths. Therefore the replacement optimum dosage of SF in the concrete in this paper was considered 12%.

  6. The adding of PPF caused an inverse influence on the tensile and compressive strengths of normal concrete and SFC.

  7. However , the adding of PPF resulted in a large decrease in compressive strength than tensile strength.

  8. the reduction in compressive and tensile strengths are directly relative to the content of fibers.

REFERENCES

  1. A. T. Hossam , E. Tahar , Influence of silica fume on compressive strength of cement paste and mortar, Cem. and Conc. Res. j., 25(1995) pp.1591-1602 .

  2. A. A. Almusallam , H. Beshr , M. Maslehuddin , O.S.B. Al-Amoudi, Effect of silica fume on mechanical properties of low quality coarse aggregate concrete, Cem. and Conc. Compos. j. , 26(2004) pp. 891-900.

  3. S. Bhanja , B. Sengupta , S. K. Kaushik , P. Kumar , Optimum silica fume content and its mode of action on concrete , ACI Mater. J., 101(2004) pp. 327-328.

  4. Nili M and Afroughsabet V. , Combined influence of silica fume and steel fibers on impact resistance and mechanical properties of concrete, Int. J. of Impact Eng. 37( 2010) pp. 879-886.

  5. Tanyildizi H. , The Effect of temperature, carbon fibers and silica fume on the mechanical properties of lightweight concretes , New Carbon Mater. J. (2008) pp. 339-344.

  6. Aktas M. , The effect of hole diameter on residual stresses and plastic region expansion in steel fiber reinforced aluminum metal-matrix laminated composite plates under transverse loading J. Reinf. Plast. Compos. 2006,25(11) pp.1149-1164.

  7. Arslan N and Ozben T. , An elastic-plastic stress analysis of a woven reinforced steel fiber thermoplastic composite cantilever beam subjected to transverse uniform loads on the upper surface . J. Reinf. Plast. Compos.2005, 24(14) pp. 1493- 1508.

  8. Ghugal YM and Deshmukh SB. Performance of alkali-resistant glass fiber reinforced concrete . J. Reinf. Plast. Compos.6( 2006 )pp. 617-630.

  9. Kumutha R and Palanichamy MS. Investigation of reinforced concrete columns confined using glass fiber-reinforced polymers. J. Reinf. Plast. Compos. 2006, 25(16)pp. 1669-1678.

  10. Mohan TP and Kanny K. Influence of nanoclay on rhe-ological and mechanical properties of short glass fiber-reinforced polypropylene composites. J Reinf. Plast. Compos. 2011, 30(2) pp.152-160.

  11. Zhang P and Li QF. Experimental study on shrinkage properties of cement stabilized macadam reinforced with polypropylene fiber. J. Reinf. Plast. Compos. 2010 ,29(12) pp.1851-1860.

  12. Niu PF, Liu BY and Wei XM. Study on mechanical properties and thermal stability of polypropylene / hemp.

  13. Balaguru PN, Shah SP. Fiber reinforced cement composites

    .New York :McGraw-Hill, Inc. 1992 -367p.

  14. N. Flores Medina , G. Barluenga , F. Hemandez-Olivares Combined effect of polypropylene fibers and silica fume to improve the durability of concrete with natural pozzolans blended cement . Construction and Building Materials j.

,2015(96) pp.556-566. mechanically and chemically activated fly ashes on mortar properties. Fuel 85 (2006) pp. 2018-2026.

Leave a Reply