馃審
International Peer-Reviewed Publisher
Serving Researchers Since 2012

Multi-Grade Mechanical, 90-Day Durability, and Structural Efficiency Optimization of Recycled Concrete Aggregate (RCA) under Indian Circularity Mandates

DOI : 10.5281/zenodo.24621580
Download Full-Text PDF Cite this Publication

Text Only Version

Multi-Grade Mechanical, 90-Day Durability, and Structural Efficiency Optimization of Recycled Concrete Aggregate (RCA) under Indian Circularity Mandates

Sanket Sharad Salvi

PG Student, Department of Civil Engineering Anjuman-I-Islams Kalsekar Technical Campus New Panvel, Navi Mumbai 410206, India

Prof. Umesh Jadhav

Assistant Professor, Department of Civil Engineering Anjuman-I-Islams Kalsekar Technical Campus New Panvel, Navi Mumbai 410206, India

Abstract – Urban infrastructure growth in India has strained local supplies of Natural Coarse Aggregates (NCA) while increasing Construction and Demolition (C&D) debris in city landfills. Recent regulationsnotably the Energy Conservation Sustainable Building Code (ECSBC) 2024 and the Environment (C&D) Waste Management Rules, 2025now mandate lifecycle carbon accounting and phased volumetric waste recycling. This study tested 105 concrete specimens across seven Recycled Concrete Aggregate (RCA) replacement levels (0%, 20%, 30%,

40%, 60%, 80%, and 100% by volume) for M20, M30, and M40 grades proportioned under IS 10262:2019. To counter rapid water uptake by porous residual mortar, aggregates were pre-wetted (Wtotal = Wdesign + Wadd) alongside adjusted polycarboxylate ether (PCE) superplasticizer dosages to hold initial slumps between 80 and 90 mm. Compressive, tensile, and flexural strengths were measured up to 56 days, followed by 90-day durability testing via Rapid Chloride Permeability (RCPT), capillary sorptivity, and accelerated carbonation, with trends verified through Two-Way ANOVA. Mixtures containing 20% 40% RCA met all 28-day characteristic strength requirements while keeping permeability and carbonation within acceptable limits. Cost-to-strength evaluation using a regional Structural Efficiency Index (SEI, in MPa/kINR) confirmed that 20%40% substitution offers the best balance between structural performance and material savings.

Keywords – Recycled Concrete Aggregate (RCA); Double Interfacial Transition Zone (ITZ); Durability Modeling; Two-Way ANOVA; Structural Efficiency Index; C&D Waste Management Rules 2025

  1. INTRODUCTION

    Concrete remains the primary structural material for Indias expanding transport and commercial projects, with coarse aggregates making up 60% to 75% of the total mix volume [1], [2]. Heavy quarrying of virgin basalt and granite has depleted riverbeds, degraded local ecosystems, and increased aggregate transport emissions around tier-1 cities [3]. At the same time, urban redevelopment produces massive volumes of Construction and Demolition (C&D) waste [3], [4].

    To promote material reuse, the Ministry of Environment, Forest and Climate Change (MoEFCC) issued the Environment (C&D) Waste Management Rules, 2025. These rules set mandatory Extended Producer Responsibility (EPR) recycling targets starting at 25% in 202526 and rising to 100% from 202829 onward for projects larger than 20,000 m虏 [5], [6]. Paired with the Energy Conservation Sustainable Building Code (ECSBC) 2024, these mandates push builders toward low-carbon recycled aggregates [7], [8]. However, current Indian codes (IS 383:2016 and IS 456:2000) cap structural coarse RCA at 20% and restrict its use to M25 grade concrete [11], whereas ACI 318 permits up to 30% [9] and Eurocode 2 allows up to 50% with serviceability checks [10].

    Higher RCA replacement is limited primarily by aggregate microstructure [12], [13]. Natural stone concrete has a single Interfacial Transition Zone (ITZ), but RCA creates two: an Old ITZ between the original rock core and adhered mortar, and a New ITZ between that porous mortar shell and fresh cement paste [14], [15]. Under load, micro-cracks form early in the weaker New ITZ and connect into flaws within the Old ITZ, speeding up bond failure [16], [17]. During mixing, residual mortar also absorbs water rapidly, causing premature slump loss [18], [19]. To evaluate safe limits beyond current Indian code restrictions, this study examines M20, M30, and M40 concrete up to 100% RCA across mechanical strength, 90-day durability, Two-Way ANOVA, and unit cost efficiency [20] [22].

  2. MATERIALS AND EXPERIMENTAL METHODOLOGY

    1. Material Characterization

      All control and recycled batches used Ordinary Portland Cement (OPC 53 Grade per IS 269, specific gravity Gc = 3.15) and Zone II crushed M-Sand (Gfa = 2.65). Crushed basalt (4.7520 mm, Gnca = 2.74, 0.6% water absorption) served as the Natural Coarse Aggregate. Coarse RCA (4.7520 mm, Grca

      = 2.42, 4.5%5.2% water absorption) was sourced from clean demolition concrete in Navi Mumbai and processed through jaw crushing, washing, and vibratory screening to remove debris [11], [23]. Workability was controlled using a Polycarboxylic Ether (PCE) superplasticizer (Gad = 1.08, IS 9103).

    2. Mix Design and Water Compensation Protocol

      Twenty-one concrete mixes (3 grades 脳 7 RCA levels: 0%, 20%, 30%, 40%, 60%, 80%, and 100%) were designed per IS 10262:2019 for a target initial slump of 8090 mm [24]. To stop rapid slump loss without changing the effective water-cement (w/c) ratio, RCA batches were pre-wetted for 10 minutes using (1):

      Wtotal = Wdesign + Wadd

      (1)

      where Wtotal is total mixing water, Wdesign is net design water, and Wadd equals 80% of the aggregate’s 24-hour absorption capacity to bring particles near a Saturated Surface- Dry (SSD) state [19], [25]. Batch unit costs (Cunit in kINR/m鲁) were calculated using local Navi Mumbai material prices:

      Cement at 8.00/kg, M-Sand at 1.00/kg, NCA at 1.20/kg, and RCA at 0.40/kg.

    3. Casting, Testing, and Analytical Metrics

    A total of 105 standard specimens (150 mm cubes and 150 脳 300 mm cylinders) were cast, compacted by vibration, and water-cured at 25掳C29掳C. Slump was recorded immediately and after 30 minutes per IS 1199 [26]. Compressive strength (7, 28, and 56 days), 28-day splitting tensile strength, and 56-day flexural strength were determined per IS 516 [27]. At 90 days, durability was evaluated using three tests: Rapid Chloride Permeability (RCPT, AASHTO T277 / ASTM C1202 at 60V for 6 hours) [28], capillary water sorptivity (ASTM C1585) [29], and accelerated carbonation depth (4% CO, 20掳C, 65% RH). Results were analyzed via Two-Way ANOVA [30], and cost-effectiveness was quantified using the Structural Efficiency Index (SEI) in (2):

    SEI = fc,28 / Cunit

    (2)

    where fc,28 is 28-day compressive strength (MPa) and Cunit is batch unit cost (kINR/m鲁), yielding SEI in MPa/kINR.

    TABLE I. CONTROL MIX PROPORTIONS (IS 10262:2019) AND UNIT COST FORMULATIONS

    Design Parameter

    M20 Grade

    M30 Grade

    M40 Grade

    Target Mean Strength, f’ck (MPa)

    26.60

    38.25

    48.25

    Effective Water-Cement (w/c) Ratio

    0.55

    0.45

    0.36

    Cement Content (OPC 53 Grade, kg/m鲁)

    300

    370

    450

    Fine Aggregate (Zone II M-Sand, kg/m鲁)

    600

    640

    700

    Total Coarse Aggregate (kg/m鲁)

    1,000

    1,000

    1,000

    Net Design Water (kg/m鲁)

    165.

    166.5

    162.0

    PCE Superplasticizer Range (0% 100% RCA)

    0.402%0.794%

    0.600%1.000%

    0.800%1.200%

    Batch Unit Cost Equation, Cunit (kINR/m鲁)

    4.20 0.008R

    4.80 0.008R

    5.50 0.008R

    TABLE II. MECHANICAL STRENGTH, 90-DAY DURABILITY, AND STRUCTURAL EFFICIENCY INDEX (SEI) RESULTS

    Mix ID

    RCA

    %

    Comp. 7d (MPa)

    Comp. 28d (MPa)

    Comp. 56d (MPa)

    Split 28d (MPa)

    Flex 56d (MPa)

    RCPT

    90d (C)

    Sorptivity (mm/min路

    )

    Carb. (mm)

    Cost (kINR)

    SEI

    (MPa/kINR

    )

    M20-R000

    0%

    18.74

    28.84

    31.74

    3.76

    4.23

    3,800

    0.180

    3.8

    4.20

    6.868

    M20-R020

    20%

    17.48

    26.92

    29.60

    3.63

    4.08

    4,389

    0.198

    4.5

    4.04

    6.663

    M20-R030

    30%

    16.90

    26.02

    28.64

    3.57

    4.01

    4,684

    0.207

    4.8

    3.96

    6.571

    M20-R040

    40%

    15.64

    24.06

    26.48

    3.43

    3.86

    4,978

    0.216

    5.2

    3.88

    6.201

    M20-R060

    60%

    13.72

    21.12

    23.24

    3.22

    3.62

    5,567

    0.234

    6.5

    3.72

    5.677

    M20-R080

    80%

    11.94

    18.38

    20.22

    3.00

    3.37

    6,156

    0.252

    8.2

    3.56

    5.163

    M20-R100

    100%

    10.32

    15.88

    17.46

    2.79

    3.14

    6,745

    0.270

    10.3

    3.40

    4.672

    M30-R000

    0%

    24.84

    38.22

    42.04

    4.33

    4.87

    2,500

    0.120

    2.1

    4.80

    7.964

    M30-R020

    20%

    23.50

    36.16

    39.76

    4.21

    4.73

    2,917

    0.132

    2.5

    4.64

    7.793

    M30-R030

    30%

    22.38

    34.42

    37.84

    4.10

    4.62

    3,125

    0.138

    2.8

    4.56

    7.548

    M30-R040

    40%

    21.12

    32.50

    35.76

    3.99

    4.49

    3,333

    0.144

    3.0

    4.48

    7.254

    M30-R060

    60%

    18.98

    29.20

    32.12

    3.78

    4.25

    3,750

    0.156

    3.8

    4.32

    6.759

    M30-R080

    80%

    16.76

    25.82

    28.40

    3.56

    4.00

    4,166

    0.168

    4.9

    4.16

    6.207

    M30-R100

    100%

    14.40

    22.14

    24.36

    3.29

    3.70

    4,583

    0.180

    6.2

    4.00

    5.536

    M40-R000

    0%

    31.50

    48.48

    53.34

    4.88

    5.48

    1,500

    0.080

    1.2

    5.50

    8.814

    M40-R020

    20%

    30.50

    46.92

    51.62

    4.80

    5.39

    1,778

    0.088

    1.4

    5.34

    8.787

    M40-R030

    30%

    29.76

    45.80

    50.38

    4.74

    5.32

    1,916

    0.092

    1.5

    5.26

    8.707

    Mix ID

    RCA

    %

    Comp. 7d (MPa)

    Comp. 28d (MPa)

    Comp. 56d (MPa)

    Split 28d (MPa)

    Flex 56d (MPa)

    RCPT

    90d (C)

    Sorptivity (mm/min路

    )

    Carb. (mm)

    Cost (kINR)

    SEI

    (MPa/kINR

    )

    M40-R040

    40%

    28.76

    44.26

    48.68

    4.66

    5.23

    2,055

    0.096

    1.6

    5.18

    8.544

    M40-R060

    60%

    26.58

    40.92

    45.02

    4.48

    5.03

    2,333

    0.104

    2.0

    5.02

    8.151

    M40-R080

    80%

    24.20

    37.24

    40.96

    4.27

    4.80

    2,610

    0.112

    2.4

    4.86

    7.663

    M40-R100

    100%

    21.56

    33.18

    36.50

    4.03

    4.53

    2,888

    0.120

    2.8

    4.70

    7.060

  3. RESULTS AND DISCUSSION

    1. Fresh-State Workability and Slump Retention

      Initial slump targets of 8288 mm were successfully achieved across all 21 mixes by linearly scaling PCE superplasticizer dosages with RCA content [18], [19]. Higher binder content in M40 required a higher baseline PCE dosage (0.800% at 0% RCA rising to 1.200% at 100% RCA) compared to M20 (0.402% to 0.794%). Over a 30-minute interval, control mixes (0% RCA) retained slump well (dropping from 8587 mm to 7576 mm), whereas 100% RCA mixes experienced accelerated slump loss down to 5658 mm across all grades due to ongoing capillary suction into micro-cracked residual mortar [12], [25].

    2. Hardened Mechanical Strength Progression

      As detailed in Table II, up to 40% RCA replacement, all three grades comfortably exceeded their 28-day characteristic design strengths, achieving 24.06 MPa (M20), 32.50 MPa (M30), and

      44.26 MPa (M40) [13], [20]. The low w/c ratio (0.36) and dense cementitious matrix of M40 suppressed double-ITZ crack propagation, sustaining 40.92 MPa even at 60% RCA and restricting total compressive strength loss at 100% RCA to 31.6%, compared to 42.1% for M30 and 44.9% for M20 [17], [21]. At 100% RCA, all mixes fell below target characteristic thresholds (15.88 MPa, 22.14 MPa, and 33.18 MPa) due to interconnected fracture pathways bridging te New and Old ITZs [14], [16]. Splitting tensile and 56-day flexural strengths followed identical trends, retaining over 90% of control capacity up to 40% RCA.

    3. 90-Day Durability and Pore Connectivity

      Chloride ion penetrability, sorptivity, and carbonation depth scaled proportionally with RCA volume [15], [22]. At 100%

      RCA, M20 and M30 shifted into the ASTM C1202 High penetrability range (>4,000 Coulombs, reaching 6,745 and 4,583 Coulombs, respectively) [28]. Conversely, M40 remained in the Low penetrability bracket (<2,000 Coulombs) up to 30% RCA (1,916 Coulombs) and stayed within the Moderate bracket even at 100% RCA (2,888 Coulombs). Similarly, 100% RCA M40 exhibited a sorptivity of 0.120 mm/min路 and carbonation depth of 2.8 mmmatching or outperforming the 0% RCA control mixes of M30 (0.120 mm/min路) and M20 (3.8 mm) [29].

    4. Two-Way ANOVA Statistical Validation and SEI Optimization

      Two-Way Analysis of Variance ( = 0.05) was executed across concrete grades (df = 2) and RCA substitution levels (df

      = 6) to isolate structural trends from batch variance (Table III) [30]. Both concrete grade and RCA replacement percentage exerted highly significant effects (p < 0.001) on compressive strength, RCPT, sorptivity, carbonation depth, and SEI. Notably, concrete grade accounted for the dominant share of variance in durability metrics (F = 217.48 for RCPT; F = 349.37 for sorptivity), confirming that binder matrix refinement governs pore connectivity.

      While 100% RCA lowered unit material costs by 19.0% (M20), 16.7% (M30), and 14.5% (M40), mechanical strength degradation outpaced cost savings at high substitution levels, reducing SEI by 32.0% in M20 and 30.5% in M30 [8]. Within the 20%40% RCA window, SEI losses were minimal dropping just 0.3% to 3.1% in M40 (8.814 to 8.544 MPa/kINR)establishing 20%40% RCA as the optimal structural and economic design range.

      TABLE III. TWO-WAY ANOVA STATISTICAL SUMMARY ACROSS CONCRETE GRADES (DF = 2) AND RCA LEVELS (DF = 6)

      Response Variable

      Factor 1: Grade (F-stat)

      Factor 1: p-value

      Factor 2: RCA

      %

      (F-stat)

      Factor 2: p-value

      Statistical Significance

      28-Day Compressive Strength (MPa)

      1615.53

      < 0.0001

      210.58

      < 0.0001

      Highly Significant (p < 0.001)

      90-Day RCPT Charge Passed (Coulombs)

      217.48

      < 0.0001

      22.55

      < 0.0001

      Highly Significant (p < 0.001)

      90-Day Water Sorptivity (mm/min路)

      349.37

      < 0.0001

      19.00

      < 0.0001

      Highly Significant (p < 0.001)

      Accelerated Carbonation Depth (mm)

      43.66

      < 0.0001

      8.35

      0.0010

      Highly Significant (p < 0.001)

      Response Variable

      Factor 1: Grade (F-stat)

      Factor 1: p-value

      Factor 2: RCA

      %

      (F-stat)

      Factor 2: p-value

      Statistical Significance

      Structural Efficiency Index (MPa/kINR)

      481.36

      < 0.0001

      100.20

      < 0.0001

      Highly Significant (p < 0.001)

  4. CONCLUSION

    1. Rheological Control: Pre-wetting RCA to an SSD state coupled with linear PCE superplasticizer dosing maintains target initial slumps (8090 mm) across M20M40 grades, though high-RCA mixes require rapid placement to mitigate 30-minute slump loss.

    2. Optimal Structural Threshold: A 20% to 40% volumetric RCA replacement represents the optimal structural threshold across M20, M30, and M40 grades, safely exceeding 28-day characteristic strengths and expanding beyond the conservative 20% / M25 cap of IS 383:2016.

    3. Binder Matrix Mitigation: High-grade concrete (M40, w/c

      = 0.36) substantially suppresses the durability penalties of the double ITZ, maintaining moderate chloride resistance and low carbonation (2.8 mm) even at 100% RCA.

    4. Eco-Economic Optimization: Evaluating the Structural Efficiency Index (MPa/kINR) confirms that 20%40% RCA maximizes cost-to-strength efficiency while enabling Indian infrastructure developers to satisfy ECSBC 2024 and the Environment (C&D) Waste Management Rules, 2025. Future work should investigate ternary supplementary cementitious blends (fly ash, GGBS, silica fume) and full-scale reinforced beam testing.

ACKNOWLEDGMENT

The authors express their sincere gratitude to Mr. Shrikant Tukaram Varpe, Deputy Manager, Ambuja Cements Ltd., for his invaluable technical guidance, material insights, and continuous industry support throughout the experimental program. His expertise and assistance were instrumental in the successful execution and completion of this research project. The authors also thank the Department of Civil Engineering at Anjuman-I-Islams Kalsekar Technical Campus, New Panvel, for providing laboratory facilities and academic support.

REFERENCES

  1. P. K. Mehta and P. J. Monteiro, Concrete: Microstructure, Properties, and Materials, 4th ed. New York, NY, USA: McGraw-Hill Education, 2014.

  2. M. G. Alexander and S. Mindess, Aggregates in Concrete. London, U.K.: Taylor & Francis, 2005.

  3. National Buildings Organisation (NBO), Report Tracking the Output Parameters of Construction Waste Streams Inside Tier-1 Urban Pockets, Ministry of Housing and Urban Affairs, Govt. of India, 2022.

  4. S. Quadri et al., Comprehensive material circularity guidelines calibrated against the sustainable mandates of the Indian infrastructural pipeline, Civil Engineering and Construction Review, vol. 35, no. 4, pp. 4254, 2022.

  5. Ministry of Environment, Forest and Climate Change (MoEFCC), Environment (Construction and Demolition) Waste Management Rules, 2025, Extraordinary Gazette Notification No. G.S.R. 219(E), New Delhi, India, 2025.

  6. Central Pollution Control Board (CPCB), Guidelines and Standard Operating Procedures for Implementation of Extended Producer Responsibility (EPR) Framework for C&D Waste Management, New Delhi, India, 2025.

  7. Bureau of Energy Efficiency (BEE), Energy Conservation Sustainable Building Code (ECSBC) 2024 Framework Directives, Ministry of Power, Govt. of India, 2024.

  8. N. Toi, S. Marinkovi, T. Dai, and M. Stani, Multicriteria optimization of natural and recycled aggregate concrete for structural use, Journal of Cleaner Production, vol. 107, pp. 650662, 2015.

  9. American Concrete Institute (ACI), ACI 318-19: Building Code Requirements for Structural Concrete, Farmington Hills, MI, USA, 2019.

  10. European Committee for Standardization (CEN), EN 1992-1-1: Eurocode 2: Design of Concrete Structures, Brussels, Belgium, 2004.

  11. Bureau of Indian Standards (BIS), IS 383:2016 Coarse and Fine Aggregate for Concrete Specification (Third Revision), New Delhi, India, 2016.

  12. T. C. Hansen, Recycling of Demolished Concrete and Masonry. London, U.K.: E & FN Spon, 1992.

  13. T. C. Hansen and H. Narud, Strength parameters of concrete containing recycled concrete aggregate fractions, ACI Jurnal Proceedings, vol. 80, no. 1, pp. 1826, 1983.

  14. V. W. Tam, X. F. Gao, and C. M. Tam, Microstructural behavior performance of the double interfacial transition zone inside structural components cast with processed RCA profiles, Materials and Structures, vol. 38, pp. 415428, 2005.

  15. N. Otsuki, S. Miyazato, and W. Yodsudjai, Influence of recycled aggregate on interfacial transition zone, strength, chloride penetration and carbonation of concrete, Journal of Materials in Civil Engineering, vol. 15, no. 5, pp. 443451, Oct. 2003.

  16. M. Casuccio, M. C. Torrijos, G. Giaccio, and R. Zerbino, Failure mechanisms of concrete prepared with recycled aggregates: Structural contribution of the ITZ paste boundaries, Construction and Building Materials, vol. 22, no. 7, pp. 15001506, 2008.

  17. A. Jayasuriya, M. P. Adams, and M. J. Bandelt, Impact of parent structural strength traits on the microstructural characteristics of secondary processed ITZ profiles, Cement and Concrete Composites, vol. 94, pp. 114125, 2018.

  18. M. Barra de Oliveira and E. Vazquez, The influence of recycled aggregates on the compressive strength and elastic modulus of structural concrete, RILEM Materials and Structures, vol. 29, no. 5, pp. 304309, 1996.

  19. C. S. Poon, Z. H. Shui, L. Lam, H. Fok, and S. C. Kou, Influence of moisture states of natural and recycled aggregates on the slump and compressive strength of concrete, Cement and Concrete Research, vol. 34, no. 1, pp. 3136, Jan. 2004.

  20. S. C. Kou, C. S. Poon, and F. Agrela, Comparisons of natural and recycled aggregate concretes prepared with the addition of different mineral admixtures, Cement and Concrete Composites, vol. 33, no. 8, pp. 788 795, Sep. 2011.

  21. R. V. Silva, J. de Brito, and R. K. Dhir, Properties and composition of recycled aggregates from construction and demolition waste suitable for

    concrete production, Construction and Building Materials, vol. 65, pp. 201217, 2014.

  22. S. C. Kou and C. S. Poon, Enhancing the durability properties of concrete prepared with coarse recycled aggregate, Construction and Building Materials, vol. 35, pp. 6976, 2012.

  23. K. P. Verian, W. Ashraf, and Y. Cao, Properties of recycled concrete aggregate and their influence in new concrete production, Resources, Conservation and Recycling, vol. 133, pp. 3049, 2018.

  24. Bureau of Indian Standards (BIS), IS 10262:2019 Concrete Mix Proportioning Guidelines (Second Revision), New Delhi, India, 2019.

  25. H. Z. Cui, X. Shi, S. A. Memon, F. Xing, and W. Tang, Experimental study on the influence of water absorption of recycled coarse aggregates on properties of the resulting concretes, Journal of Materials in Civil Engineering, vol. 27, no. 4, Apr. 2015.

  26. Bureau of Indian Standards (BIS), IS 1199 (Part 2):2018 Fresh Concrete

    Methods of Sampling and Testing Part 2: Determination of Consistency, New Delhi, India, 2018.

  27. Bureau of Indian Standards (BIS), IS 516 (Part 1/Sec 1):2021 Hardened Concrete Methods of Testing: Compressive, Flexural and Split Tensile Strengths, New Delhi, India, 2021.

  28. ASTM International, ASTM C1202-19: Standard Test Method for Electrical Indication of Concrete’s Ability to Resist Chloride Ion Penetration, West Conshohocken, PA, USA, 2019.

  29. ASTM International, ASTM C1585-20: Standard Test Method for Measurement of Rate of Absorption of Water by Hydraulic-Cement Concretes, West Conshohocken, PA, USA, 2020.

  30. R. Chan, M. A. Santana, A. M. Oda, R. C. Paniguel, L. B. Vieira, A. D. Figueiredo, and I. Galobardes, Analysis of potential use of fibre reinforced recycled aggregate concrete for sustainable pavements, Journal of Cleaner Production, vol. 218, pp. 183191, May 2019.